In FDM and FFF 3D printing, the infill pattern largely determines mechanical load capacity, part weight and print time. While conventional grid patterns are prone to the dreaded nozzle scraping under shear forces and fast print head movements, modern 3D geometries such as Gyroid and Adaptive Cubic offer almost isotropic strength in all three spatial axes (X, Y, Z). In this practical guide, 3D Bäckerei Berlin compares the most common infill structures for functional industrial and prototype parts – including guideline values for infill density and wall lines, specific slicer settings for PrusaSlicer, OrcaSlicer, Bambu Studio and Cura, and an overview of typical defects.

1. What infill is for: supporting top layers, keeping walls apart

In FDM printing, the inside of a part is almost never filled solid. An infill of 100 % multiplies print time and weight and, because of the greater thermal shrinkage, increases the risk of warping. Instead, an infill structure takes on two clearly defined tasks:

  • Scaffold for the top layers: The infill acts as a base so that the horizontal upper layers do not sag into the cavities. If the pattern is too coarse or the density too low, holes and ripples appear in the surface (“pillowing”).
  • Absorbing compressive, shear and torsional forces: It prevents thin outer walls from buckling, distributes point loads into the body of the part and keeps the walls apart under bending.

A look at lightweight construction mechanics helps here: in parts subjected to bending, the highest tensile and compressive stresses occur in the outermost fibres – exactly where the wall lines are. The infill acts like the core of a sandwich panel: it absorbs shear stresses and keeps the load-bearing skins apart. This leads to the most important rule of this guide: the strength of an FDM part comes mainly from the walls; the infill stabilises them. You can read more in our guide to wall thickness & perimeters in 3D printing.

2. Structural analysis: 2D patterns (Grid, Triangles) vs. true 3D patterns (Gyroid, 3D Honeycomb)

Classic 2D infill patterns (e.g. Grid, Triangles, Rectilinear) repeat the same paths in every layer and are simply “extruded” in the Z direction. This saves computing time when slicing, but means that the part has very different strength properties along the Z axis than in the X and Y directions (anisotropy). Grid and Triangles have a second problem: the filament paths cross each other at the same height at the intersections. Small material build-ups form there, which the hot nozzle scrapes over at high speeds – leading to rattling, nozzle wear or even skipped steps.

True 3D patterns such as Gyroid, Cubic or 3D Honeycomb change their geometry continuously with each layer and form a spatial wave or cell lattice that absorbs forces from all directions. Gyroid has no fixed crossing points within a layer. Rectilinear (Lines) is a special case: although it is a 2D pattern, it prints only parallel lines in each layer, with the direction alternating by 90° from layer to layer – so there are no collisions within a layer.

Using our online calculator (order 3D printing), we manufacture your assemblies with an optimally calculated internal structure.

3. Infill matrix: strength, print speed & nozzle collision risk

Comparison of the mechanical and printing properties of common slicer infill patterns. The density ranges are approximate guideline values common in practice for functional parts and are no substitute for testing the specific part:

Infill patternIsotropic strength (XYZ)Print speed / flowNozzle collision riskTypical density (guideline)Best use
GyroidExcellent (uniform in all axes)Medium – high (continuous)No risk (no crossing points)12–25 %Mechanical functional parts, TPU dampers, vibration damping
Honeycomb (Honeycomb / 3D Honeycomb)Very high (excellent compressive stiffness)Slow (many changes of direction)Low15–30 %Lightweight load-bearing structures, sandwich panels, vertically loaded supports
GridMedium (weak in torsion, anisotropic)Very fast (straight lines)High (scraping at intersections)15–20 %Quick concept models without dynamic loads
Rectilinear (Lines)Moderate (direction-dependent)MaximumNone (no crossings within a layer)15–25 %Flat covers, housing lids, visible patterns
CubicVery good (tilted 3D cube cells)FastMedium (occasional crossings)15–25 %Sturdy all-round parts with good top-layer support
Adaptive CubicHigh near surfaces, economical in the coreFastLow10–20 %Large solid prototypes with maximum material savings
Cross HatchGood (combines speed and stability)Very fastLow10–20 %High-speed series production on Bambu / Voron
LightningVery low (supports upwards only)Extremely fastNone10–20 %Purely visual and decorative models, figurines, architectural models

4. Why Gyroid is the superior pattern for technical functional parts

The Gyroid pattern is based on a triply periodic minimal surface (TPMS). It is available in PrusaSlicer, OrcaSlicer, Bambu Studio and Cura and offers unique physical advantages:

  • Even force distribution: Loads in the X, Y and Z directions are transferred homogeneously into the part without a preferred axis of weakness. This is why Gyroid often needs a slightly lower density than Grid to achieve comparable stiffness.
  • Open, interconnected channels: All cavities are connected to one another. This makes Gyroid ideal for flow-through filter bodies, floats and buoyancy bodies, and for parts that are subsequently filled with epoxy resin or PU foam – the casting medium spreads without trapped air pockets.
  • Gentle on the print head: Smooth sine curves without crossing points eliminate nozzle scraping; skipped steps and torn-off filament crumbs inside the part are avoided.
  • Ideal for flexible materials: With TPU and other flexible filaments, Gyroid flexes evenly in all directions without forming kinks. The density (around 10–30 %) lets you fine-tune the perceived hardness of a TPU damper.

The catch: The constant curved movements create many small acceleration events. On printers without input shaping, the frame can vibrate noticeably with Gyroid, and on fast machines it is often the acceleration rather than the nominal speed that limits the pace. Remedies include reduced infill acceleration, enabled input shaping (Klipper, Bambu firmware) and the automatic path smoothing of modern slicers such as OrcaSlicer and Bambu Studio.

5. Honeycomb, Cubic, Adaptive Cubic, Lightning & Rectilinear: which pattern when?

Honeycomb and 3D Honeycomb

Classic 2D Honeycomb extrudes hexagonal prisms vertically upwards. This produces very high compressive stiffness in the Z direction (along the prism walls) – ideal for pressure plates and vertically loaded support columns. Across that direction, the pattern is considerably more compliant. 3D Honeycomb, available in PrusaSlicer and OrcaSlicer, behaves in a more spatially balanced way. Both variants involve many changes of direction and are therefore among the slowest patterns. Cura has no Honeycomb; Tri-Hexagon comes closest to it.

Cubic and Adaptive Cubic

Cubic creates cube cells tilted by 45° and is a fast all-rounder with good support for horizontal top surfaces. Adaptive Cubic (PrusaSlicer, OrcaSlicer, Bambu Studio; comparable to “Cubic Subdivision” in Cura) densifies the infill only near the walls and top layers and leaves large cells in the core. For large-volume parts this noticeably saves print time and filament without degrading top-layer quality. How much you save depends heavily on the geometry – for compact, thin-walled parts the effect is small.

Lightning infill

Lightning builds tree-like structures that grow only where top layers need to be supported; the rest of the model stays hollow. For figurines, architectural and display models, this is the fastest and most economical solution. Lightning is unsuitable for functional parts, as it carries practically no load. With Lightning, plan for additional top layers so that the surface does not sink in.

Rectilinear, Grid and Triangles

Thanks to its collision-free paths, Rectilinear remains a fast pattern for flat housing covers. Grid and Triangles do offer decent in-plane stiffness, but should be avoided on fast printers (as a guideline, from around 150 mm/s infill speed) – here Gyroid, Cubic or Cross Hatch are the better choice.

6. Infill density vs. wall lines (perimeters): where real strength comes from

In engineering design, the rule of thumb is: wall lines (perimeters) provide strength, infill supports the top surfaces. A typical beginner’s mistake is to crank the infill density up to 60–100 % to get a strong part.

  • Strength increases less than proportionally with infill density: from around 30–40 %, the gain flattens out significantly, while material consumption and print time keep rising almost linearly. Our guide Calculating print time: slicer estimates and filament consumption shows how to estimate print time and filament usage realistically in advance.
  • Additional wall lines, on the other hand, act precisely in the outer fibre, where bending and torsional stresses are highest. A part with 4–5 walls and 15–25 % Gyroid is generally stiffer in bending and torsion than one with 2 walls and 50–60 % infill – while using less material.
  • High infill percentages also increase heat input and shrinkage, which aggravates warping with ABS, ASA and nylon.

The following overview summarises proven starting values (guideline values for a 0.4 mm nozzle):

ApplicationWall linesInfillTop/bottom layers
Display and demonstration models210–15 % Lightning or Adaptive Cubic5 top / 4 bottom
Standard parts, housings, brackets2–312–18 % Gyroid or Cubic4–5 top / 3–4 bottom
Mechanically stressed functional parts4–620–25 % Gyroid or Cubic5–6 top / 4–5 bottom
Fibre-reinforced parts (PA-CF, PETG-CF)4–525–30 % Gyroid5–6 top / 4–5 bottom
Flexible TPU parts2–310–30 % Gyroid (depending on the desired hardness)4 top / 3 bottom

Besides walls and infill, the orientation in the build volume also determines load capacity, because the layer boundaries remain the weakest point of an FDM part. You will find advice on this in our articles on part orientation in 3D printing and layer adhesion.

7. Adaptive infill & modifiers: increasing density precisely at load points

With modern slicers, you do not have to fill the entire model uniformly. Two tools are particularly effective:

  • Gradient or adaptive infill: Cura offers “Gradual Infill Steps” – the density increases in steps towards the top layers, while the core remains more loosely filled. In PrusaSlicer, OrcaSlicer and Bambu Studio, Adaptive Cubic plays a similar role.
  • Local modifiers: Place cylindrical or box-shaped modifier bodies around screw holes, bearing seats or heat-set inserts and increase the infill density or wall count there – up to 100 % infill in the area of the screw connection. In PrusaSlicer, OrcaSlicer and Bambu Studio this is called a “Modifier” or “Height range modifier”, in Cura “Infill Mesh” or “Per Model Settings”. Our guide to modifiers in 3D printing explains how to create such areas in the individual slicers and which starting values have proven effective.

This keeps the part light and quick to print, while the zones that actually bear loads are made solid. For holes and threads, the number of walls around the hole is also more important than the infill density next to it.

8. Slicer settings: PrusaSlicer, OrcaSlicer, Bambu Studio & Cura

The functions are available in all common slicers, but go by different names:

FunctionPrusaSlicerOrcaSlicer / Bambu StudioCuraGuideline
Pattern & densityFill pattern / Fill densitySparse infill pattern / densityInfill Pattern / Infill Densitysee table above
Infill only every nth layerCombine infill every n layersInfill combinationInfill Layer ThicknessTotal thickness ≤ approx. 75 % of nozzle diameter
Infill/wall overlapInfill/perimeters overlapInfill/Wall overlapInfill Overlap Percentage15–30 %
Infill line widthInfill extrusion widthLine width → Sparse infillInfill Line Width110–140 % of the nozzle (0.45–0.55 mm with 0.4 mm)
Connect infill endsLength of the infill anchorSparse infill anchor lengthConnect Infill Linesenable
Local reinforcementModifierModifierInfill Mesh / Per Model Settingsaround holes & threads
  1. Infill combination: The outer contours are printed at a fine layer height, the infill only every second layer at double height – depending on the model, this saves a considerable amount of print time. Make sure that the combined layer thickness does not exceed roughly three quarters of the nozzle diameter: with a 0.4 mm nozzle, 2 × 0.15 mm works reliably, with a 0.6 mm nozzle 2 × 0.2 mm.
  2. Wider infill lines: A line width of 110–140 % of the nozzle diameter improves the bonding of the infill paths to one another and to the inner walls.
  3. Check the overlap: An infill/wall overlap of 15–30 % securely fuses the infill to the inner perimeters. Values that are too high show up as bulges on the outer wall. Our article on infill overlap has the details.
  4. Connect infill ends: Anchored or connected infill lines prevent loose start and end points at the inner walls.
  5. Mind the volumetric flow: Infill is usually printed at the highest speed. If the set speed exceeds the hotend’s maximum melt flow, the infill is under-extruded and brittle. Limit the infill speed via the maximum volumetric flow rate.

9. Infill beyond FDM: hollowing in SLA printing

In resin printing (SLA/MSLA), the internal structure behaves completely differently: solid resin parts generate high peel forces on the FEP film and consume a lot of photopolymer. Larger models are therefore hollowed out (hollowing, as a guideline with a wall thickness of 2.0–2.5 mm) and, if necessary, stiffened with an internal lattice structure. Hollowed parts absolutely require at least two drain holes near the build plate so that liquid residual resin can drain away, no suction-cup effect occurs and the interior can be reached during washing and post-curing. There is no classic infill pattern as in an FDM slicer.

10. Defects & solutions

DefectCauseSolution
Rattling, scraping noises, layer shift in the infillNozzle scrapes over crossing points (Grid, Triangles)Switch to Gyroid, Cubic or Rectilinear; reduce infill speed
Holes and ripples in the top layer (pillowing)Density too low, Lightning, too few top layersIncrease top layers to a total thickness of at least 0.8–1.0 mm; raise density or use Adaptive Cubic
Gap between infill and wallOverlap too small, infill too fastInfill/wall overlap to 15–30 %; connect infill ends; reduce speed
Infill shows through on the outer wallToo few walls or overlap too highAt least 3 wall lines; reduce overlap; print walls before infill
Brittle, crumbly infillUnder-extrusion due to excessive volumetric flowLimit infill speed to the max. flow rate; check temperature
Strong vibrations with GyroidMany acceleration changes due to curved pathsReduce infill acceleration; enable input shaping
Warping despite (or because of) 100 % infillHigh heat input and shrinkageLower the density and increase walls instead; heat the build chamber
Part breaks along the layersWeak layer adhesion, unfavourable orientation – not an infill problemChange print orientation; adjust temperature and cooling

11. Industrial prototype and small-batch production in Berlin

In our Berlin production facility, we define the infill, wall thicknesses and print orientation for each part individually according to its load case – from quick demonstration samples to highly stressed functional parts in FDM 3D printing. For development teams, we produce assemblies from engineering plastics through to carbon-fibre-reinforced high-performance polymers as part of rapid prototyping and small-batch production.

Want a functional part made with an optimal internal structure?

Upload your STL or 3MF file, choose material and quantity – the price is calculated instantly.

Upload your part and get an instant price

12. Frequently asked questions (FAQ)

What infill density is best for standard functional parts?

For most technical parts, 15 to 25 % Gyroid or Cubic infill combined with 4 to 5 wall lines offers a good balance of strength and weight. For simple housings and brackets, 12 to 18 % with 2 to 3 walls is often sufficient.

Do you have to print with 100 % infill for maximum strength?

Usually not. Beyond about 30 to 40 % infill, strength increases only slightly, while print time, weight and the risk of warping continue to rise. Additional wall lines increase bending and torsional stiffness far more effectively.

Why does Grid infill make loud scraping noises while printing?

Grid infill crosses the printed paths at the same layer height. At high speeds, the print head scrapes over these intersections, which can lead to nozzle wear or skipped steps. Gyroid, Cubic or Rectilinear solve the problem.

Which infill pattern is best for TPU and flexible filaments?

Gyroid, because it stretches and compresses evenly in all directions without forming kinks. The infill density lets you set the hardness of the part precisely.

Which infill pattern uses the least filament?

Lightning creates support structures only beneath the top layers and leaves the rest hollow. It is suitable for display and decorative models, but not for load-bearing functional parts.

When is Adaptive Cubic worthwhile instead of Gyroid?

For large-volume prototypes and housings where material and print time matter most. Adaptive Cubic densifies the infill only near the surfaces and saves material in the core; for evenly loaded functional parts, Gyroid remains the safer choice.

What does the “infill every second layer” setting achieve?

The infill is printed at double layer height while the outer walls remain fine. This saves print time without any visible loss of quality. The combined layer thickness should not exceed about 75 % of the nozzle diameter.

How do I order robust functional parts in Berlin?

Upload your CAD files to our online price calculator, choose material and quantity and get a price instantly. We define the infill, wall thicknesses and orientation to suit the load case.


⚡ 3D Bäckerei Berlin
3D printing with 24h express from Berlin
Calculate price online ➔
📱 3D file on your PC?
Send yourself the direct link via Telegram or WhatsApp and upload your STEP/STL file comfortably on your computer: