Press-fit joints that are too tight, rough top surfaces with grooves or small holes between the top-most lines often share the same cause: the printer is not delivering exactly the amount of plastic the slicer calculated. Just a few per cent of over- or under-extrusion is enough to make fits bind or walls lose strength. The solution is a two-level calibration: first the mechanical E-steps (or rotation distance in Klipper) of the extruder, then the material-specific extrusion factor (Flow Rate, Flow Ratio or Extrusion Multiplier) in the slicer. In this guide, 3D Bäckerei shows you how to determine both values cleanly using callipers, a hollow cube and the calibration tests in OrcaSlicer and Bambu Studio – and how to tell flow problems apart from other sources of error.
Table of contents
- 1. E-steps vs. flow rate: why hardware & software are calibrated separately
- 2. Step by step: the 100 mm method for E-steps & rotation distance
- 3. Preparation: filament diameter, temperature & drying
- 4. The hollow cube test: checking wall thickness with callipers
- 5. Two-stage flow test in OrcaSlicer & Bambu Studio
- 6. Typical flow values: PLA, PETG, ABS/ASA, TPU & carbon nylon
- 7. Over- or under-extrusion? Reading the symptoms correctly
- 8. Flow, dimensional accuracy & fits
- 9. Defects & solutions
- 10. Frequently asked questions (FAQ)

1. E-steps vs. flow rate: why hardware & software are calibrated separately
In FDM printing, the slicer calculates for every line how many millimetres of filament the extruder needs to push so that line width, layer height and line length produce the correct volume. Whether this calculation ends up being right depends on two fundamentally different quantities that are often confused:
- E-steps or rotation distance (hardware): In the firmware, the E-steps define how many motor steps are needed to move 1 mm of filament. Klipper describes the same thing the other way round via the rotation distance – the length of filament per full motor revolution. The value depends only on the gearing, the drive gear diameter and the microstepping, and applies equally to all filaments.
- Flow rate / extrusion factor (slicer): A multiplier in the filament profile, 1.00 or 100 % by default. It compensates for material-specific effects: deviations in the actual diameter, how much the melt swells after leaving the nozzle (die swell), the hardness of the filament and how deeply the drive gear bites into it.
The separation matters because otherwise an incorrect hardware value would have to be corrected in every filament profile as well. If, for example, you “fix” E-steps that are 5 % out via the flow, you have to compensate for this error again with every new material and soon lose track. The sensible order is therefore:
- Check E-steps or rotation distance (once, and after any modifications to the extruder).
- Make sure the filament diameter, printing temperature and dryness of the material are right.
- Determine the flow rate for each filament and save it in the profile.
- Only then set dynamic parameters such as Pressure Advance or Linear Advance and the maximum melt capacity.
2. Step by step: the 100 mm method for E-steps & rotation distance
The 100 mm method works equally well with Marlin, Klipper and RepRapFirmware. You will need callipers or an accurate ruler, a fine marker and access to the printer console.
Step 1: Heat the hotend and mark the filament
Heat the nozzle to the usual printing temperature of the loaded material, around 200–215 °C for PLA. Most firmware blocks the extruder below a minimum temperature. Measure 120 mm along the filament from the extruder inlet and make a fine mark there.
Step 2: Slowly extrude 100 mm
Switch to relative extrusion and feed 100 mm at low speed, for example with M83 followed by G1 E100 F60 (1 mm/s). The low speed is crucial: when feeding quickly, back pressure builds up in the nozzle, the drive gear slips and the result is distorted. On Bowden printers, you can alternatively carry out the test with the tube disconnected directly at the extruder.
Step 3: Measure the remaining length
Measure the remaining distance from the extruder inlet to the mark. If it is exactly 20 mm, the E-steps are correct. If it is more than 20 mm, too little filament was fed; if it is less, too much. The length actually fed is 120 mm minus the remaining length. Ideally, repeat the measurement two or three times and calculate with the average.
Step 4: Calculate and save the new value
Marlin: New E-steps = (current E-steps × 100) / length actually fed. M503 shows the current value in the M92 line. Example: currently 93.0 steps/mm, 95 mm was fed. Calculation: 93.0 × 100 / 95 = 97.89 steps/mm. The value is set with M92 E97.89 and saved permanently with M500.
Klipper: New rotation distance = current rotation distance × (length actually fed / 100). Because the rotation distance is a distance per revolution, the value becomes smaller in the case of under-extrusion. Enter it in the [extruder] section of printer.cfg and restart the firmware.
Closed systems: On printers such as Bambu Lab or newer Prusa models, the extruder values are set at the factory and are not intended to be adjusted in normal operation. Here you calibrate the flow directly in the slicer.
If the result deviates significantly or varies between measurements, the problem usually does not lie in the firmware: check the extruder spring tension, worn or dirty drive gears and a partially clogged nozzle before changing any values.
3. Preparation: filament diameter, temperature & drying
Before you determine the flow, the boundary conditions that will also apply to the actual print should be right. Otherwise you will calibrate in an error that originates elsewhere.
- Filament diameter: Slicers assume 1.75 mm by default. However, the volume per millimetre of filament grows with the square of the diameter. If a spool actually measures 1.72 mm, it mathematically delivers around 3.4 % less material ((1.72 / 1.75)² ≈ 0.966). Measure the diameter at several points and in two directions offset by 90°. If the average deviates significantly, enter it as the filament diameter in the profile instead of hiding the deviation in the flow.
- Printing temperature: Calibrate the flow at the temperature you will later print at. Temperature and speed change the viscosity of the melt and therefore how it flows in the nozzle.
- Dry filament: Damp PETG, nylon or TPU forms steam bubbles when melted. The lines become porous and look under-extruded, even though the flow is correct.
- Moderate speed: Do not print the test at the performance limit of the hotend. If the maximum volumetric melt capacity is exceeded, under-extrusion occurs that has nothing to do with the flow factor.
4. The hollow cube test: checking wall thickness with callipers
The classic measuring method compares the printed wall thickness with the target value from the slicer. It is independent of the slicer and well suited to finding a starting value for new materials.
- Create the test piece: A cube with an edge length of about 20–30 mm, printed in vase mode (Spiralize Outer Contour) with exactly one outer wall, no infill and no top layers.
- Set a fixed line width: Set the outer wall width to a fixed value, e.g. 0.45 mm with a 0.4 mm nozzle. Automatic width calculations should be disabled for this test.
- Set the flow to the current value: Note down the flow entered in the filament profile so that the calculation is correct.
- Measure: Measure all four walls at roughly half height using the flat jaws, not the tips, and without applying pressure – otherwise you will compress the plastic. Take the average.
- Calculate: New flow = current flow × (target wall thickness / measured wall thickness).
Worked example: Target 0.45 mm, measured average 0.47 mm, current flow 1.00. New flow = 1.00 × 0.45 / 0.47 ≈ 0.957. So in the slicer you enter approximately 0.96 or 96 %.
The method has limitations you should be aware of: the wall is not perfectly flat but shows the ripples of the individual layers. The callipers therefore pick up the peaks and tend towards a slightly too large value. In addition, a measuring deviation of just 0.01–0.02 mm on a 0.45 mm wall amounts to around 2–4 %. A variant with two walls (target e.g. 0.90 mm) halves the relative measuring error, but additionally depends on how much the lines overlap. For fine-tuning, the visual test in the next section is therefore often more meaningful.
5. Two-stage flow test in OrcaSlicer & Bambu Studio
OrcaSlicer and Bambu Studio include ready-made flow tests in the Calibration menu. They do not assess the wall thickness but the top surface – precisely where over- and under-extrusion become visible in everyday printing. You don’t need any tools for this, just your eyes and fingertips.
- Pass 1 (coarse test): The slicer generates nine test plates with deviations from −20 % to +20 % in 5 % steps relative to the current filament profile. After printing, run your finger over the surfaces. Choose the plate that feels smoothest: without palpable grooves or gaps (too little flow) and without rough, raised ridges (too much flow).
- Calculate the new value: New flow = old flow × (100 + modifier) / 100. Example: old flow 0.98, best plate −5. New flow = 0.98 × 95 / 100 = 0.931. Enter this value in the filament profile before starting Pass 2.
- Pass 2 (fine test): A second set of plates in 1 % steps refines the result. The calculation is the same; the result is entered to two or three decimal places.
Newer OrcaSlicer versions also offer a more compact test variant with fine increments in a single run. When assessing, make sure you have even light from the side: raking light makes grooves and ridges much more visible than light from above. Bambu Studio distinguishes between the flow rate test and the Flow Dynamics Calibration – the latter determines the pressure advance factor, not the extrusion factor.
Where to enter the value in the slicer:
| Slicer | Parameter | Note |
|---|---|---|
| OrcaSlicer / Bambu Studio | Filament settings → Flow ratio | Built-in calibration tests in the Calibration menu |
| PrusaSlicer | Filament Settings → Filament → Extrusion multiplier | Save the value per filament profile |
| Cura | Material → Flow as a percentage | Separate flow values for walls, infill and first layer possible |
The two methods complement each other: the hollow cube provides a measurable starting value, while the top surface test assesses the result under real printing conditions. A flow that looks perfect on the top surface is usually the better choice for visible parts than a mathematically exact value with a slightly rough surface.
6. Typical flow values: PLA, PETG, ABS/ASA, TPU & carbon nylon
The following ranges are guide values that frequently occur after a clean E-step calibration. They are no substitute for your own measurement – manufacturer, colour, nozzle and printer all shift the optimum.
| Material | Flow (guide value) | Typical with too much flow | Typical with too little flow |
|---|---|---|---|
| PLA / PLA+ | approx. 0.95–1.00 | Rough top surfaces, dimensions too large | Small holes next to the outer walls |
| PETG | approx. 0.92–0.97 | Material builds up on the nozzle, blobs | Weaker layer bonding, open top surfaces |
| ABS / ASA | approx. 0.93–0.98 | Nozzle scrapes across infill and top surfaces | Porous walls, lower strength |
| TPU (95A and softer) | approx. 1.00–1.08 | Jams in the extruder, filament buckles | Spongy, incomplete walls |
| PA-CF / PETG-CF | approx. 0.95–1.02 | Rough edges, increased nozzle wear | Pores in the part, gaps in the infill |
A few relationships explain the differences: PETG swells comparatively strongly after leaving the nozzle and tends to ooze, which is why a slightly reduced flow often gives cleaner results. Soft TPU is compressed between the drive gears and responds sluggishly to pressure changes; a marginally increased flow and, above all, a low printing speed help. You can find out more in the material profile for flexible TPU. Fibre-reinforced filaments are stiffer and hardly slip on the drive gear; however, they wear down brass nozzles, which means the effective nozzle diameter – and with it the flow behaviour – changes over time.
Colour and additives also play a role: heavily pigmented variants, such as white with a high titanium dioxide content, as well as silk filaments often behave differently from the natural colour of the same line. Within a single product line from the same manufacturer, one profile is usually sufficient; when changing manufacturer, using new colours with unusual additives or seeing a visibly different print result, a quick check test is worthwhile.
7. Over- or under-extrusion? Reading the symptoms correctly
Before you adjust the flow, it pays to take a close look at the defect. Many symptoms look like an incorrect extrusion factor but have a different cause.
- Over-extrusion (flow too high): The nozzle ploughs through the top layer, the top surface feels rough and grooved, outer walls are thicker than in the CAD model, and holes and slots become too narrow. Edges and corners look bulging, and the nozzle may audibly scrape across the material during infill.
- Under-extrusion (flow too low): Gaps or small holes remain between the top layer lines, walls look matt and porous, and lines do not fully touch each other. Layer adhesion suffers, and parts break more easily along the layers under load.
Typical mix-ups:
- Bulges only at corners, otherwise clean walls: This is more of a pressure advance issue than a flow problem, because pressure builds up in the nozzle when decelerating.
- Under-extrusion only at high speed or on large infill areas: The hotend cannot melt enough material to keep up. More flow will not help here; what helps is a lower volumetric flow or a more powerful hotend.
- Increasing under-extrusion during a print: Often an incipient clog, heat creep or an overheated extruder motor.
- Crackling, bubbles or hissing while printing: Moisture in the filament.
- Problems only in the first layer: This is usually down to the Z offset, not the flow; the procedure is described in the guide to first layer calibration.
8. Flow, dimensional accuracy & fits
A correctly calibrated flow is a prerequisite for dimensionally accurate parts, but it is not the only adjustment. If the outer dimensions are correct after calibration but holes are still too small, this is due to geometry: STL files represent circles as polygons, and at tight radii the melt is pushed inwards. You do not compensate for these effects via the flow, but via hole or XY compensation in the slicer and by designing in suitable clearances.
- Hole compensation: Deliberately enlarging inner contours by a small amount – as a guide value around 0.1 mm – helps with holes for screws and pins. The exact value depends on the material, diameter and printer and should be determined with a test part.
- Wall order: If the inner walls are printed first and then the outer walls, the outer wall rests against an already solid line and is usually closer to the target dimension.
- Top surfaces: For visible top faces, the calibrated flow rate can be combined with ironing. Here the hot nozzle passes over the top layer a second time with greatly reduced flow (by default around 10–15 % in many slicers).
How shrinkage, XY size compensation and hole tolerances interact is explained in the guide to dimensional accuracy and XY compensation. For prototypes with fits in rapid prototyping, we match material, profile and tolerances to the specific part, including for projects from Berlin Mitte and Charlottenburg. Urgent parts can be requested via our express 3D printing in Berlin. If the CAD model for a replacement part is missing, the original can be digitised using our 3D scanning service.
Dimensionally accurate parts without doing the calibration yourself?
Upload your STL or 3MF file, choose the process, material and quantity – the price is calculated online instantly.
9. Defects & solutions
| Defect | Cause | Solution |
|---|---|---|
| Rough, grooved top surface, nozzle scrapes | Flow too high | Run flow test Pass 1 and 2, lower the value in the filament profile |
| Gaps and holes between the top layer lines | Flow too low, too few top layers | Calibrate flow, check the number of top layers |
| 100 mm test gives widely varying results | Drive gear slipping, extruded too fast, nozzle partially clogged | Feed at 1 mm/s, check spring tension and drive gears, clean the nozzle |
| New filament suddenly prints differently | Different diameter or different formulation | Measure and enter the diameter, create a separate profile with its own flow |
| Bulges only at corners, walls otherwise clean | Pressure build-up when decelerating | Calibrate Pressure Advance or Linear Advance, do not change the flow |
| Under-extrusion only at high speed | Maximum melt capacity of the hotend exceeded | Limit volumetric flow in the slicer, reduce speed or moderately increase temperature |
| Porous walls, crackling and bubbles | Damp filament | Dry the filament and store it dry, then check the flow again |
| TPU jams in the extruder | Speed too high, too much flow, long filament path | Print slowly, keep flow moderate, use a direct drive extruder if possible |
| Outer dimensions correct, holes too small | Polygonisation and melt displacement at radii | Use hole or XY compensation instead of lowering the flow |
| Flow value drifts over weeks with CF filament | Wear of a brass nozzle caused by fibres | Use a hardened nozzle, replace a worn nozzle and recalibrate |
10. Frequently asked questions (FAQ)
Do I need to recalibrate the E-steps every time I change filament?
No. E-steps or rotation distance depend only on the mechanics of the extruder and apply to all materials. You should recheck the value after modifying or replacing the extruder, fitting new drive gears or changing the microstepping. Differences between filaments are compensated for exclusively via the flow in the slicer.
Do I need to readjust the flow for every spool of filament?
For spools from the same product line and the same manufacturer, a profile calibrated once is usually sufficient. When changing material, for example from PLA to PETG, switching to a different manufacturer or using colours with unusual additives such as silk filaments, a quick check test makes sense.
What is the difference between flow rate and pressure advance?
The flow rate determines the basic amount of material delivered along the entire line. Pressure Advance or Linear Advance, on the other hand, controls the dynamic pressure in the nozzle when accelerating and decelerating, so that no bulges form at corners and no thin spots appear after changes of direction. The flow is calibrated first, then pressure advance.
Why does TPU print with under-extrusion even though PLA works perfectly?
Soft TPU is compressed between the drive gears and in the filament path and responds sluggishly to pressure changes. As a result, less material arrives than calculated at higher speeds. What usually helps most is a significantly lower printing speed, supplemented by a slightly increased flow and a filament path that is as short and tight as possible.
Which method is more accurate: the hollow cube or the flow test in the slicer?
Both have their strengths. The hollow cube provides a measurable figure but is sensitive to measuring errors, because just a few hundredths of a millimetre amount to several per cent. The top surface test in OrcaSlicer or Bambu Studio assesses the result under real conditions. In practice, the cube is suitable for a starting value and the slicer test for fine-tuning.
How does the filament diameter affect the flow?
The volume delivered grows with the square of the diameter. A filament measuring 1.72 mm instead of 1.75 mm mathematically delivers around 3.4 per cent less material. Measure the diameter at several points and, if there is a significant deviation, enter the average in the profile instead of compensating for the difference via the flow.
How can I recognise under-extrusion on a finished part?
Typical signs are gaps between the lines of the top layer, matt and porous walls, visible gaps between the outer and inner walls and weak layer adhesion. If the defect only occurs at high speed, the melt capacity of the hotend is more likely to be the cause than a flow that is too low.
Why are printed holes too small despite a calibrated flow?
Circles are approximated as polygons in STL files, and at tight radii the nozzle pushes the melt slightly inwards. This geometric effect cannot be fixed via the flow. Instead, use hole or XY compensation in the slicer and design suitable clearances into the model.
Do I need to calibrate the E-steps on Bambu Lab printers?
As a rule, no. On Bambu Lab and other closed systems, the extruder values are set at the factory. There, the flow is calibrated in the slicer using the flow rate test. The Flow Dynamics Calibration in Bambu Studio, on the other hand, determines the pressure advance factor and does not replace flow calibration.