Table of contents
- 1. Why threaded inserts? Plastic threads vs. brass inserts
- 2. CAD design rules: undersize, taper, chamfer & reservoir
- 3. Design table: hole dimensions & chamfers for M2 to M8
- 4. The temperature guide: insertion temperatures for PLA, PETG, ABS, PA-CF & PC
- 5. Tools: soldering irons, insert tips & jigs
- 6. Slicer optimisation: wall lines, modifiers & print orientation
- 7. Step by step: professional insertion without tilting
- 8. 5 practical tips for pull-out strength & clean threads
- 9. Special cases: SLA resin, nuts via print pause & stainless steel inserts
- 10. Common defects & solutions
- 11. Have parts made with inserts already installed
- 12. Frequently asked questions (FAQ)
Threads cut directly into plastic or printed in place quickly reach their physical limits in professional FDM 3D printing: after just a few screwing cycles the thermoplastic wears out, screws strip or the part cracks along the layer lines.

3D printing threaded inserts heat-set inserts installation Berlin
The proven solution for strong, reusable screw connections in printed parts is thermal threaded inserts made of brass (heat-set inserts). Installed correctly, they withstand high pull-out and torque loads and allow clean connections with metric machine screws. In this guide, 3D Bäckerei from Berlin summarises all the key design dimensions, temperatures, tools, slicer settings and typical defects – from the hole in CAD to the fully assembled part.
1. Why threaded inserts? Plastic threads vs. brass inserts
Compared with square nuts in slot-in pockets or self-tapping screws, tapered or cylindrical knurled threaded inserts offer clear advantages:
- High pull-out strength: The heat-softened polymer flows into the knurl grooves and, once cooled, forms a solid positive lock. Opposing knurl patterns (diamond or herringbone) secure the insert against both pull-out and rotation at the same time.
- Many screwing cycles: Metal metric threads (DIN / ISO) can be assembled very many times and tightened to a defined torque without wearing the plastic.
- Compact footprint: No side pockets for nuts are needed – ideal for slim enclosures and fixtures in industrial jig and fixture construction.
- Precise position: The thread sits exactly on the designed axis, regardless of the dimensional accuracy of printed threads.
Fastening methods compared
Heat-set inserts are not always the only sensible option. The following overview helps you choose the right connection for your printed part:
| Method | Strengths | Weaknesses | Suitable for |
|---|---|---|---|
| Printed / cut thread | No additional parts, quick | Wears out after a few cycles, low load capacity with small threads | Large threads, connections that are rarely undone |
| Self-tapping plastic screws | Simple, inexpensive | Spreading forces can split the boss along the layers, limited cycles | One-off assembly, lids, covers |
| Nut in slot-in pocket | High load capacity, standard parts | More space required, nut can fall out or spin | Thick parts, large threads from M6 |
| Cold press-in / expansion insert | No heat needed, also suitable for resin | Lower pull-out values, risk of cracking with knurled inserts without heat | SLA resin parts, lightly loaded connections |
| Bonded insert | For non-meltable materials | Curing time, adhesive may get into the thread, usually weaker than heat-set | Thermosets, SLA resin, repairs |
| Ultrasonic insertion | Very fast, repeatable | Expensive equipment, process development required | Industrial series, injection-moulded parts |
| Heat-set insert (heat) | Strong hold, many screwing cycles, compact, can be done with a soldering iron | Requires exact hole size and temperature, thermoplastics only | Enclosures, fixtures, functional parts in FDM and SLS |
How printed and cut threads work in detail, and when they are sufficient, is explained in our guide Threads in 3D printing.
2. CAD design rules: undersize, taper, chamfer & reservoir
The quality of an insert connection is already decided in CAD. Follow the rules below and you will get a straight fit, a clean surface and enough material in the knurl grooves.
Hole undersize
The hole must be smaller than the outer diameter of the knurling so that the displaced plastic can flow into the grooves. As a rule of thumb, use an undersize of about 0.2–0.4 mm relative to the outer knurl diameter. Too little undersize gives a weak positive lock; too much displaces so much material that it bulges over the surface or is pushed into the thread.
Tapered hole (approx. 8° included angle)
Many manufacturers of tapered inserts recommend a slightly tapered hole with an upper diameter d1 and a smaller lower diameter d2 – corresponding to an included angle of around 8°. The advantage: the insert centres itself when positioned and is easier to guide straight. Cylindrical holes also work, provided the insert is cylindrical and guided with a jig.
Lead-in chamfer
A chamfer of 0.5–1.0 mm × 45° (up to 1.5 mm for M5 and larger) at the hole entrance makes it easier to start the insert straight and takes up some of the displaced material. This prevents a bulge from forming around the insert.
Reservoir below the insert
Design the hole 1.0–1.5 mm deeper than the length of the insert. This cavity catches excess plastic and prevents it from being pushed into the thread from below. Through holes do not have a reservoir; in that case the insert must be guided so that it does not slip through.
Wall thickness of the screw boss
Enough material must remain around the insert so that the boss does not crack during insertion or under load. As a guideline, the wall around the hole should be at least half the outer diameter of the insert (about 2 mm for M3, i.e. a boss outer diameter of around 8–9 mm). For highly loaded connections, a wall of 1.5 to 2 times the hole radius makes sense.
Load direction and insertion direction
Ideally, design the part so that the screw pulls the insert into the part when tightened – i.e. insert it from the side opposite the screw connection. The flange or end face of the insert then bears against the plastic, rather than the knurling alone carrying the load.
3. Design table: optimal hole dimensions & chamfers for M2 to M8
The following values are guideline values for common tapered brass inserts of standard length. Since outer diameter and length vary between manufacturers, the datasheet for your insert always takes precedence. The ranges cover the differences between typical designs.
| Thread | Hole Ø top (d1) | Hole Ø bottom (d2) | Hole depth | Min. wall around boss | Lead-in chamfer |
|---|---|---|---|---|---|
| M2 | 3.0–3.2 mm | 2.8–3.0 mm | Insert length + 1.0 mm | 1.6 mm | 0.5 mm × 45° |
| M2,5 | 3.4–3.8 mm | 3.2–3.5 mm | Insert length + 1.0 mm | 1.8 mm | 0.5 mm × 45° |
| M3 (standard) | 4.0–4.4 mm | 3.7–4.0 mm | Insert length + 1.0–1.5 mm | 2.0 mm | 0.8 mm × 45° |
| M4 | 5.4–5.7 mm | 5.0–5.3 mm | Insert length + 1.0–1.5 mm | 2.5 mm | 1.0 mm × 45° |
| M5 | 6.4–6.8 mm | 6.0–6.4 mm | Insert length + 1.5 mm | 3.0 mm | 1.2 mm × 45° |
| M6 | 8.0–8.6 mm | 7.6–8.1 mm | Insert length + 1.5 mm | 3.5 mm | 1.5 mm × 45° |
| M8 | 9.6–10.2 mm | 9.2–9.7 mm | Insert length + 1.5 mm | 4.0 mm | 1.5 mm × 45° |
Important for dimensional accuracy: In FDM, printed holes usually come out slightly smaller than in CAD because the outer contour of the perimeters spreads inwards. Before a production run, print a small test plate with several hole diameters in 0.1 mm steps and choose the hole in which the insert, under light pressure, stays put by itself at about a third of its depth. Alternatively, correct systematically using hole compensation in the slicer – for details, see the guide Tolerances & fits in 3D printing.
4. The temperature guide: insertion temperatures for PLA, PETG, ABS, PA-CF & PC
As a rule of thumb, set the soldering tip to roughly the printing temperature up to around 20 °C above it. Too cold, and the insert has to be forced in – this creates stress and tilting. Too hot, and the plastic becomes runny, bulges up, discolours or degrades. Heat transfer depends heavily on the soldering iron, tip size and insert size, so start at the lower end of the range and work your way up.
| Material | Soldering tip temperature (guideline) | Cooling before loading | Note |
|---|---|---|---|
| PLA / Tough PLA | 200–230 °C | approx. 1 min | Little pressure needed, PLA softens quickly and bulges up |
| PETG | 230–250 °C | 1–2 min | Flows cleanly, tends to string at the tip |
| ABS / ASA | 240–265 °C | approx. 2 min | Good bond, material stays tough |
| PA / PA-CF (carbon fibre nylon) | 260–300 °C | 2–3 min | Dry parts beforehand to avoid bubbles; very strong hold |
| PC / PC blends | 280–310 °C | approx. 3 min | Powerful soldering iron needed, guide evenly |
| PEEK / PEI | approx. 340–380 °C | several minutes | Only with a high-temperature station and special tips |
The cooling times are also guideline values: only load or screw into the insert once the plastic around the knurling has fully solidified again. With large inserts (M6, M8) and thick bosses, this takes correspondingly longer.
5. Tools: soldering irons, insert tips & jigs
For individual inserts, a temperature-controlled soldering iron is all you need. What matters is not expensive equipment, but a suitable tip and straight guidance.
- Temperature-controlled soldering iron: Compact USB-C or mains-powered soldering irons (e.g. Pinecil, TS100/TS101) or soldering stations (e.g. Weller, Ersa) with adjustable temperature. A stable temperature is important so that the tip does not cool down significantly on contact with the cold brass.
- Heat-set tips: Stepped brass or copper tips for each thread size, with a guide pin that engages in the insert. They transfer heat evenly and prevent plastic from being pushed into the internal thread. Normal pointed soldering tips are unsuitable.
- Guide pin / alignment screw: A screw or pin turned into the insert shows immediately whether it is sitting straight and helps with alignment.
- Insertion jig: A small drill stand or a jig with a linear, spring-loaded guide holds the soldering iron exactly vertical. The spring limits the pressing force so that heat rather than force does the work – ideal for series production.
- Flattening block: A flat metal block (aluminium, steel) for pressing the still-warm insert flush.
6. Slicer optimisation: wall lines, modifiers & print orientation
A common mistake: the insert is installed in a part with only 2 wall lines and 15 % grid infill. The knurling then partly grips into empty space, and the boss cracks during cooling or tightening. The remedy is a modifier that reinforces only the area around the insert, without printing the entire part more solidly. Observe the following slicer rules:
- Wall lines (perimeters): At least 4 to 6 wall lines around the hole – with a 0.4 mm nozzle, that is around 1.6–2.4 mm of solid material. The area around the insert should consist of solid material as far as possible. Why more walls often achieve more than high infill is explained in our guide to wall thickness & perimeters.
- Local modifiers: Instead of printing the whole part solid, place cylindrical regions with 100 % infill or additional walls around the screw bosses. In PrusaSlicer via “Add modifier”, in OrcaSlicer and Bambu Studio via “Add modifier” with their own wall and infill values, in Cura via “Per Model Settings” with the option “Modify settings for overlaps”.
- Bottom and top layers: Provide at least 4–5 bottom layers under a blind-hole floor so that the insert does not break through during insertion.
- Hole compensation: If holes consistently come out too small, XY hole compensation (OrcaSlicer/Bambu Studio “X-Y hole compensation”, Cura “Hole Horizontal Expansion”) corrects this specifically without changing the outer dimensions.
- Print orientation: Holes with a vertical axis (in the Z direction) come out round and dimensionally accurate. Horizontal holes become slightly oval and the insert presses across the layers – here the risk of delamination is considerably higher. Where possible, plan the part orientation so that the insert axes are vertical.
7. Step by step: professional insertion without tilting
- Prepare: Fit the matching heat-set tip, set the temperature according to the material and let the soldering iron heat up fully. Secure the part firmly with the hole pointing vertically upwards.
- Position the insert: Place the threaded insert straight into the lead-in chamfer, narrow end first. Tapered inserts centre themselves in the tapered hole.
- Apply the soldering iron: Insert the guide pin of the tip into the insert and let it rest lightly for a few seconds until the brass is heated through.
- Gentle vertical pressure: Let the heat do the work. After a few seconds, the insert sinks in evenly. If you have to push hard, the iron is too cold or the hole is too small.
- Stop just short of the surface: Pull the soldering iron out vertically about 0.5 mm before reaching the surface – do not tilt it, otherwise the insert will be pulled crooked.
- Press flat: Immediately press the still-hot insert flush with, or about 0.1–0.2 mm below, the part surface using a flat metal block and hold for a few seconds. This way it sits perfectly flat and the mating part rests cleanly on the plastic.
- Let it cool: Leave the part to rest for 1–3 minutes depending on the material, without loading the insert.
- Check: Turn a screw in by hand. It must run smoothly and sit straight. Residue in the thread can be carefully removed with a tap of the same size.
8. 5 practical tips for maximum pull-out strength & clean threads
- Special heat-set tips instead of soldering tips: Stepped heat-set tips prevent molten plastic from being pushed into the internal thread and keep the insert axially aligned.
- Correcting a tilted insert: Reinsert the tip, reheat for 2–3 seconds and straighten the insert using a screw turned into it as a lever. Then press it flat. If that does not work, pull the insert out while warm using a screw and use a new hole or a new part.
- Use a drill stand as a pressing aid: Clamp the soldering iron in a small drill stand or a spring-loaded jig – this gives you a repeatable 90° fit without tilting.
- Clearance below the insert (reservoir): Always design the hole 1.0–1.5 mm deeper than the insert. This cavity catches displaced plastic and keeps the thread clean from below.
- Think about the load path: Preferably install inserts from the side opposite the screw connection, so that the screw pulls them into the part. For highly loaded connections, choose longer inserts or a larger thread size – the contact area with the plastic determines the hold more than the brass itself.
Pull-out strength vs. over-torque
When designing, it is worth distinguishing between two failure modes: pull-out strength (the axial force at which the insert is pulled out of the plastic) and over-torque (the torque at which the insert spins in the boss). Insert length, wall thickness, dense material around the hole and an insertion direction in which the screw pulls the insert in all help against pull-out. Opposing knurling and completely filled grooves help against spinning. Actual forces depend heavily on the insert, material, wall structure and temperature; for safety-critical connections you should therefore carry out your own tensile and torque tests with the actual print profile.
9. Special cases: SLA resin, nuts via print pause & stainless steel inserts
SLA and resin parts
Cured photopolymers from SLA printing are thermosets and do not melt – a heat-set insert would only burn or crack the resin. For resin parts, bonded threaded bushings (two-component epoxy) or special expansion or press-in inserts are suitable. SLS parts made of PA12, on the other hand, work well with heat-set inserts.
Embedding nuts via a print pause
If a nut is to disappear completely into the material, it can be inserted during printing: the printer pauses at the appropriate layer height, the nut is placed and then printed over. This way it can neither fall out nor spin. Our guide Print pause in 3D printing describes how this works in practice.
Stainless steel inserts and bonding
Stainless steel inserts are available for corrosive or food-related environments. They conduct heat less well than brass and therefore need a little more time or a higher temperature. Additional bonding is not necessary with correctly installed brass inserts and carries the risk of adhesive running into the thread. A pulled-out insert can be refitted with two-component epoxy as an emergency fix, but usually does not reach its original strength. Use a tough, gap-filling adhesive for this and keep the thread clear with a greased screw.
10. Common defects & solutions
| Defect | Cause | Solution |
|---|---|---|
| Insert sits crooked | Pressed freehand, soldering iron tilted when pulled out, no chamfer | Reheat and align with a screw; in future use a drill stand/jig and a lead-in chamfer |
| Plastic in the thread | Too much undersize, no reservoir, pointed soldering tip, too hot | Re-cut with a tap; make the hole 1.0–1.5 mm deeper, use a heat-set tip, lower the temperature |
| Bulge / material swells over the surface | Hole too small, temperature too high, no chamfer | Enlarge the hole, 0.5–1.0 mm chamfer, press flat with a metal block |
| Screw boss cracks | Wall too thin, too few perimeters, pressed in cold, hole axis across the layers | Wall ≥ half insert Ø, 4–6 wall lines, insert at a higher temperature, reorient the part |
| Insert spins when tightened | Hole too large, knurl grooves not filled, too much torque | Smaller hole, insert with opposing knurling, limit tightening torque |
| Insert protrudes above the surface | Hole too shallow, floor printed too thick, not pressed flat | Depth = insert length + 1.0–1.5 mm; press flush while warm with a metal block |
| Insert can be pulled out | Inserted too cold, infill instead of solid material around the hole, load pulls against the insertion direction | Modifier with 100 % infill, check temperature, install insert from the opposite side |
| Bubbles, discolouration or odour | Temperature too high, damp material (especially PA) | Reduce temperature, dry nylon parts beforehand |
11. Have parts made with inserts already installed
For enclosures, brackets and fixtures, 3D Bäckerei can supply parts ready for assembly with heat-set threaded inserts on request – from single parts to small-batch production. Urgent assemblies are also possible with express 3D printing in Berlin. Simply specify the thread size, insert type and position when ordering; the holes should be designed according to the rules above.
Want an enclosure or fixture printed with threaded inserts?
Upload your STL or 3MF file, choose material and quantity – the price is calculated instantly.
12. Frequently asked questions (FAQ)
Can threaded inserts also be pressed in cold?
Knurled heat-set inserts should not be pressed in cold: this creates high internal stresses and can split the screw boss along the layer lines. For cold insertion there are special press-in or expansion inserts, although these usually achieve lower pull-out values.
What hole diameter do I need for an M3 insert?
For common tapered M3 inserts, the guideline hole diameter is 4.0–4.4 mm at the top (d1) and 3.7–4.0 mm at the bottom (d2), with a depth of insert length plus 1.0–1.5 mm. The manufacturer’s datasheet is authoritative; a test plate with several diameters shows the best size for your printer.
What soldering iron temperature is right for PLA and PETG?
As a guideline, roughly the printing temperature up to around 20 °C above it: for PLA approx. 200–230 °C, for PETG approx. 230–250 °C. Start at the lower end and only increase if the insert does not sink in under light pressure.
How much pull-out force can a heat-set M3 insert withstand?
That depends heavily on the insert design, material, wall thickness and insertion direction. Correctly installed inserts in solid material hold considerably more than printed threads; it is often the plastic around the boss that fails rather than the insert. For critical applications, you should carry out your own tensile tests with your material and print profile.
From which direction should the screw force act?
Ideally, the insert is installed from the rear so that the screw pulls it into the plastic housing when tightened, instead of pulling it out. The insert then bears against the material and the knurling is relieved.
What should I do if the insert is crooked?
Reinsert the heat-set tip, reheat for 2–3 seconds and straighten the insert with a screw turned into it, then press it flat with a metal block. If it is badly tilted, pull the insert out while warm and use a new hole.
Do heat-set inserts work in SLA resin parts?
No. Cured resin is a thermoset and does not melt. For SLA parts, use bonded threaded bushings with two-component epoxy or special expansion or press-in inserts. SLS parts made of PA12, on the other hand, are well suited to heat-set inserts.
Should inserts also be glued in?
With correctly installed inserts in thermoplastics this is not necessary, and adhesive can run into the thread. Bonding makes sense for non-meltable materials or to repair a pulled-out insert, but then usually does not achieve the strength of a heat-set connection.