Polypropylene is found in caps with living hinges, laboratory containers, car interior trim and battery boxes. The plastic is lightweight, tough, extremely chemical-resistant and absorbs virtually no water – properties that also make it attractive for FDM printing. At the same time, PP is considered one of the most stubborn filaments: it adheres to almost no print surface, shrinks considerably as it cools and is prone to warping. Anyone who wants to print polypropylene therefore needs to master adhesion and cooling behaviour above all. In this guide we show how we process PP, glass-fibre-reinforced PP-GF and PP-CF in our professional 3D printing service in Berlin, which print surfaces work, which parameters have proven themselves and how you can avoid the typical mistakes.

1. What makes polypropylene special

Polypropylene is a semi-crystalline thermoplastic from the polyolefin group. With a density of only 0.90 g/cm³, it is the lightest common engineering plastic – it floats on water. Its glass transition temperature lies below freezing point, and its melting range is around 160 to 165 °C. For functional parts, these properties are particularly interesting:

  • Chemical resistance: PP withstands acids, alkalis, alcohols and many solvents. That is why it is used for laboratory supplies, containers, pump housings and parts that come into contact with cleaning agents.
  • Fatigue resistance: PP tolerates a very large number of bending cycles. This makes it the classic material for living hinges and snap fits.
  • Low moisture absorption: Unlike PA, PC or PETG, PP absorbs hardly any water. Dimensions and strength remain stable even in humid environments.
  • Low surface energy: The same property that makes PP so resistant is the reason for its poor adhesion – on the print bed, but also when bonding and painting.
MaterialDensityPrinted tensile strength (XY)Elongation at breakChemical resistanceTendency to warp
PLA1.24 g/cm³50–60 MPalowlowlow
PETG1.27 g/cm³45–50 MPamediummediumlow
ABS1.04 g/cm³35–45 MPamediumlow to mediumhigh
PP0.90 g/cm³20–30 MPavery highvery highhigh
PP-GF1.00–1.05 g/cm³30–40 MPamediumvery highmedium
Guide values for typical FDM filaments; properties of printed parts depend on orientation, parameters and manufacturer.

PP is therefore not a material for maximum stiffness, but for tough, lightweight and resistant parts. Where heat resistance and impact strength matter more, our guide to polycarbonate printing is the better place to start. You can find an overview of all materials on our 3D printing materials page.

2. The right print surface

When printing polypropylene, the print surface determines success or failure. PP only adheres reliably to surfaces that are themselves made of polyolefin or specially coated for it. On glass, smooth PEI and powder-coated spring steel, the part usually comes loose after just a few layers.

Proven surfaces

  • PP packing tape: Clear polypropylene packing tape is the cheapest and most reliable solution. Apply the strips without overlaps or air bubbles and degrease them with isopropyl alcohol. At a bed temperature of 60 to 85 °C, PP adheres to it very well.
  • PP sheet: A thin polypropylene sheet, fixed to the bed with clips or double-sided tape. Adhesion is excellent, often even too strong – the part fuses to the sheet if the temperature and contact pressure are too high.
  • Special adhesion promoters: Liquid adhesives for PP, applied to PEI or glass, form a thin layer to which PP adheres and from which it releases again after cooling.
  • Coated build plates: Some manufacturers offer spring steel plates with a PP-compatible coating. They are convenient, but wear out faster with frequent PP use.

First layer

For PP, the first layer should be squished slightly more than with PLA. A Z offset reduced by 0.02 to 0.04 mm and a first layer width of 120 to 150 per cent increase the contact area. The first layer speed is 15 to 20 mm/s. With a PP sheet, the opposite applies: leave a little more gap here so that the part does not fuse inseparably.

3. Controlling shrinkage and warping

As a semi-crystalline plastic, PP shrinks by 1.5 to 2.5 per cent as it cools – significantly more than amorphous materials such as ABS or PETG. As it crystallises, the material contracts and builds up internal stresses that lever the corners off the bed. Anyone who wants to print polypropylene therefore combines several measures:

  • Brim or mouse ears: 5 to 10 mm brim for parts with corners; for large parts, discs at the corners are often sufficient.
  • Enclosure: A closed chamber at 35 to 50 °C slows down cooling. Higher chamber temperatures bring hardly any benefit with PP, because the material stays well above its glass transition anyway.
  • Glass fibre reinforcement: PP-GF shrinks considerably less and barely warps. For dimensionally accurate parts, it is often the better choice than unreinforced PP.
  • Design: Avoid large, closed surfaces, round off corners and replace thick cross-sections with ribs.
  • Scaling: For fits, compensate for shrinkage in the slicer with 100.5 to 101.5 per cent and verify it on a test piece.

We describe the physical principles of warping and further countermeasures in our guide to warping with ABS, ASA and nylon.

4. Parameters by PP type

PP filaments differ considerably depending on polymer type and filler. Homopolymers are stiffer but shrink more; copolymers are tougher and usually easier to print. The following table summarises the starting values we use to print polypropylene:

TypeNozzleBedPart cooling fanSpeedPrint surfaceSpecial feature
PP copolymer220–240 °C60–85 °C20–50 %30–60 mm/sPP tape, PP sheetmost common filament type, tough
PP homopolymer230–250 °C80–100 °C10–30 %30–50 mm/sPP sheet, adhesivestiffer, greater shrinkage
PP-GF (glass fibre)230–260 °C80–100 °C10–30 %40–80 mm/sPP tape, adhesivehardened nozzle, barely any warping
PP-CF (carbon fibre)230–260 °C80–100 °C10–30 %40–80 mm/sPP tape, adhesivehardened nozzle, high stiffness
Starting values from our workshop; the information in the respective manufacturer’s data sheet takes precedence.

Unreinforced PP is soft and tends to buckle in the extruder. If you want to print unreinforced polypropylene, a direct drive extruder with a short, tightly guided filament path is therefore much more reliable than a Bowden system. Retraction is short: 0.5 to 1.5 mm on direct drive extruders at 25 to 35 mm/s. Drying PP is only necessary if the filament visibly forms bubbles or has been stored unsealed for a long time; 4 hours at 60 to 65 °C is usually enough.

Cooling in moderation

Unlike ABS or PC, PP needs a certain amount of cooling, otherwise overhangs and small details sag. Too much airflow, however, increases warping. 20 to 50 per cent fan speed from the third layer onwards and a minimum layer time of 10 to 15 seconds for small cross-sections have proven effective.

Applications where PP excels

  • Living hinges and closures: Thin PP hinges survive thousands of bending cycles. We describe the design rules in our guide to living hinges in 3D printing.
  • Containers and laboratory parts: Holders, funnels and adapters for cleaning and process chemicals.
  • Lightweight automotive and housing parts: Clips, covers and ducts where weight and toughness count.
  • Food-related applications: PP base materials are often approved for food contact, but for printed parts the filament, printing process and surface must be assessed together. Background information can be found in our article on food-safe 3D printing in accordance with EU 10/2011.

5. Settings in PrusaSlicer, OrcaSlicer and Cura

Generic PP profiles are available in all three slicers, but they are often too optimistic regarding speed and cooling. If you want to print polypropylene, it is best to create your own filament profile and save it with the print surface used in its name.

PrusaSlicer

  • Filament → Temperature: First layer 5 °C hotter than the rest; bed temperature to suit the surface, 70 to 85 °C for PP tape.
  • Filament → Cooling: Fan off for the first two to three layers, then 20 to 50 per cent; set “Enable fan if layer print time is below” to 15 s.
  • Filament → Filament Overrides: Retraction length 0.8 to 1.2 mm, speed 30 mm/s.
  • Print Settings → Skirt and brim: Brim 6 to 10 mm; for large parts, use the brim type “Outer brim only”.
  • Print Settings → Advanced: For fits, use “XY Size Compensation” instead of blanket scaling.

OrcaSlicer

  • Filament → Basic information: Enter a density of 0.90 g/cm³ so that weight and cost are correct. Set the shrinkage compensation (“Shrinkage”) in the filament profile to the measured value, around 98.5 to 99.5 per cent.
  • Filament → Cooling: Set “No cooling for the first” to 3 layers; fan 20 to 50 per cent, up to 70 per cent for overhangs.
  • Build plate: Store a separate bed temperature for each plate type. For a plate you have taped yourself, choose a custom plate type.
  • Calibration: Run a temperature tower and flow test once for each new PP filament, as copolymers from different manufacturers vary greatly.

Cura

  • Material: Cura includes a generic PP profile that serves as a starting point. Check and adjust density, printing temperature and bed temperature.
  • Cooling: Set “Regular Fan Speed at Height” to about 0.6 mm so that the fan ramps up slowly.
  • Adhesion: Brim of 8 mm; enable “Brim Only on Outside” so that no hard-to-remove edges form on the inside.
  • Special Modes: Enable the “Draft Shield” if the printer has no enclosure.
  • Travel: Short retraction distance and “Combing” within the model to avoid strings on the surface.

6. Step-by-step guide

This is how we proceed when we print polypropylene – from the print surface to the finished part:

  1. Prepare the print surface: Apply PP tape without wrinkles or fix a PP sheet in place, and degrease with isopropyl alcohol.
  2. Check the printer: Direct drive extruder with tight filament guidance, clean nozzle, and a hardened nozzle for PP-GF and PP-CF.
  3. Create a profile: Temperatures and fan as per the table, brim 6 to 10 mm, first layer 15 to 20 mm/s, retraction 0.5 to 1.5 mm.
  4. Compensate for shrinkage: Print a cube with 50 mm edges, measure it and store the scaling or shrinkage factor in the profile.
  5. Run a test print: Print a small test piece with corners and a living hinge and check it for adhesion, warping and hinge function.
  6. Print the part: Watch the first layer, close the enclosure and avoid draughts.
  7. Remove the part: Let the bed cool to room temperature; with PP tape, peel the part off with the tape and replace the tape if it is damaged.

7. Defects & solutions

These are the problems we encounter most often when printing polypropylene:

DefectCauseSolution
First layer does not stickUnsuitable surface (glass, smooth PEI)Use PP tape, a PP sheet or PP adhesive; degrease the surface
Corners lift after a few millimetresCrystallisation shrinkage, draughtsEnlarge the brim, use an enclosure, reduce the fan, use PP-GF
Part has fused to the PP sheetBed temperature too high, too much contact pressureLower the bed temperature, increase the Z offset, switch to PP tape
Filament buckles in the extruderSoft material, Bowden system, too much tensionDirect drive extruder, reduce tension, lower speed
Sagging overhangs and detailsToo little coolingFan at 40–70 % for overhangs, increase minimum layer time
Holes and fits too smallShrinkage not compensatedSet the shrinkage factor in the profile, measure a test piece
Layers separate when bentNozzle too cold, fan too strongTemperature +5–10 °C, reduce the fan, increase line width

Three rules solve most of the problems:

  • Always use a PP-compatible print surface – parameters alone are no substitute for adhesion.
  • Plan for shrinkage in fits right from the start.
  • Allow for the low surface energy during post-processing: adhesives and paints only adhere to PP after pre-treatment. We describe suitable methods in our guide to bonding 3D printed parts.

8. Conclusion

Printing polypropylene is worthwhile wherever chemical resistance, low weight and fatigue resistance are required – from living hinges and laboratory parts to lightweight automotive clips. The key lies not in exotic hardware, but in the right print surface, controlled cooling and consistent compensation for shrinkage. Unreinforced PP demands patience; PP-GF and PP-CF are considerably more dimensionally accurate and often the better choice for technical parts. For recurring parts, we document the approved parameters for each filament batch so that small series remain reproducible too.

Need PP parts manufactured? Calculate your price now

Would you like to have polypropylene parts printed without optimising print surfaces and profiles yourself? Upload your STL or STEP file to our 3D printing cost calculator and receive an indicative price instantly. For PP-GF, living hinges and series parts, we will advise you personally – find out more about our 3D printing services.

9. Frequently asked questions (FAQ)

What does polypropylene stick to in 3D printing?

Reliably to PP tape, PP sheets, special PP adhesives and build plates coated for this purpose. PP generally does not adhere to glass or smooth PEI.

What nozzle temperature does PP filament need?

Depending on the type, 220 to 260 °C: PP copolymers around 220 to 240 °C, homopolymers as well as PP-GF and PP-CF 230 to 260 °C.

Does PP filament need to be dried?

Usually not, as PP absorbs hardly any moisture. Only if bubbles form or after very long unsealed storage, about 4 hours at 60 to 65 °C is sufficient.

How much does polypropylene shrink?

Unreinforced PP shrinks by about 1.5 to 2.5 per cent. Glass-fibre-reinforced PP-GF shrinks considerably less and barely warps.

Can I print polypropylene if my printer has a Bowden extruder?

With stiff PP-GF often yes; with soft unreinforced PP it is difficult, because the filament buckles in the tube. A direct drive extruder is much more reliable.

Is PP suitable for living hinges?

Yes, PP is the classic material for them. Printed hinges should be oriented so that the extrusion lines run across the hinge.

Can PP parts be bonded or painted?

Only to a limited extent. Because of the low surface energy, special polyolefin adhesives, primers or plasma or flame treatment are required.

Are printed PP parts food-safe?

The base material is often approved, but for printed parts the filament, additives, printing process and rough surface must be assessed together. A general statement is not possible.


⚡ 3D Bäckerei Berlin
3D printing with 24h express from Berlin
Calculate price online ➔
📱 3D file on your PC?
Send yourself the direct link via Telegram or WhatsApp and upload your STEP/STL file comfortably on your computer:
✓ Link copied to clipboard!