Table of contents
- 1. What is ironing? The physical principle of hot smoothing
- 2. Applications: when is ironing worthwhile in B2B & prototyping?
- 3. Prerequisites: preparing top layers, flow & nozzle
- 4. The core parameters: flow, speed, line spacing, inset & pattern
- 5. Configuration in PrusaSlicer, OrcaSlicer, Bambu Studio & Cura
- 6. Ironing calibration test: finding the right ironing flow
- 7. Material analysis: which filament delivers the best results?
- 8. Defects & solutions
- 9. Limits of ironing & sensible alternatives
- 10. Time vs. quality: is ironing worth it?
- 11. Frequently asked questions (FAQ)

1. What is ironing? The physical principle of hot smoothing
In FDM/FFF 3D printing, horizontal top surfaces (top layers) consist of plastic strands laid down side by side. Even with a well-calibrated flow and fine layer heights, fine, tangible ridges and nozzle tracks remain visible between the lines. On visible parts, housing lids, display bezels or flat seating surfaces, this line structure is both visually and haptically distracting. Ironing (also known as surface smoothing) is a slicer feature that noticeably smooths exactly these top layers directly during the printing process – without sanding, filling or painting.
Once the regular last solid layer has been laid down, the hot nozzle passes over the same surface a second time – at the same Z height, but with very tight line spacing (typically 0.10 to 0.15 mm with a 0.4 mm nozzle). Only a tiny amount of material is extruded, typically 10 to 15 % of the regular extrusion volume. Three effects work together:
- Thermal plasticising: The flat end face of the nozzle melts the microscopic peaks of the top layer and presses them flat.
- Micro-extrusion: The small additional flow fills the valleys between the original lines so that no open gaps remain.
- Overlap: Because the line spacing is much smaller than the nozzle diameter, the nozzle passes over every point several times. The result is a homogeneous surface – from satin matt to glossy depending on the material – without visible individual lines.
2. Applications: when is ironing worthwhile in B2B & prototyping?
In industrial projects and for visible parts, the feel of a component often determines its perceived quality. Ironing is always worth considering when large, flat, upward-facing surfaces are visible or functionally relevant:
- Visible front panels & electronics housings: Device fronts and lids receive a uniform finish without distracting line patterns.
- Mating surfaces & mounting planes: Flat contact surfaces for screw connections sit more evenly because the ridge peaks have been levelled.
- Seating surfaces for seals: Flat gaskets made of silicone or EPDM sit much better on an ironed surface than on a ridged one. For critical applications, however, whether the joint is actually tight must still be checked case by case – ironing is no substitute for machined face finishing.
- Type plates, logos & scales: Multicolour lettering on the top layer looks sharper and higher in contrast on a smoothed surface.
- Sliding surfaces: In guide grooves or slider elements, a smoothed surface noticeably reduces snagging and chattering.
- Flat housing lids in small batches: Time-consuming sanding, priming and painting are no longer needed for many one-offs and small batches.
Ironing makes less sense for purely functional internal parts, for components with almost exclusively sloped or curved surfaces, and for parts that will be painted or coated anyway.
3. Prerequisites: preparing top layers, flow & nozzle
Ironing can only smooth what is already closed. It does not hide holes, under-extrusion or “pillowing” (bulges above the infill). A separate guide explains how to avoid holes and bumps in top layers. Before fine-tuning, therefore, check the following basics:
- Enough top layers: 4–5 solid top layers, or a top shell thickness of around 0.8 mm, have proven to be a good basis (guideline value). With too few top layers, the melted material sinks into the cavities of the infill.
- Suitable layer height: 0.16 to 0.20 mm is ideal for the last top layer before ironing. Very thick layers leave deeper ridges that the low ironing flow can no longer fill completely.
- Calibrated flow: A top layer that is already over- or under-extruded cannot be rescued by ironing. First calibrate the flow rate or extrusion multiplier for the filament in question.
- Monotonic top fill: A monotonic top pattern (Monotonic / Monotonic Line) lays all lines in the same direction and provides a more even starting surface than a randomly alternating rectilinear pattern.
- Clean, intact nozzle: Adhering plastic residue is dragged across the surface during ironing. Clean the nozzle with a brass brush before printing; with PETG, a silicone sock helps prevent material build-up.
- Dry filament: Moist material tends to form bubbles and strings, which show up as matt spots or craters after ironing.
4. The core parameters: flow, speed, line spacing, inset & pattern
A good ironing result comes from fine-tuning just a few variables. The following values are guideline values for a 0.4 mm nozzle and serve as a starting point for your own tests:
| Parameter | Guideline value (0.4 mm nozzle) | Physical effect |
|---|---|---|
| Ironing Flow | 10 % – 15 % | Delivers just enough plastic to fill the ridges. Too little: open ridges and holes. Too much: beads and scaly edges. |
| Ironing Speed | 15 – 40 mm/s, on fast printers with PLA sometimes up to approx. 60 mm/s | Determines the contact time for heat transfer. Too fast: the surface is not sufficiently plasticised. Very slow: higher risk of heat creep. |
| Line Spacing | 0.10 – 0.15 mm | Must be much smaller than the nozzle diameter so that the ironing lines overlap and no edges remain visible. |
| Ironing Inset | 0.2 – 0.4 mm | Stops the nozzle short of the outer contour so that displaced polymer is not pushed over the edge. |
| Ironing Pattern | Rectilinear/Zig Zag; Concentric for round surfaces | Linear patterns produce even light refraction; concentric patterns avoid kinks from direction changes on round lids. |
| Ironing Type (scope) | Top surface only or all top surfaces | Determines whether only the highest surface or every upward-facing surface (e.g. steps, ledges) is ironed. |
Consider flow and line spacing together
Ironing flow and line spacing influence each other: with tighter spacing, the nozzle covers more lines per area and therefore deposits more material overall. If you reduce the spacing from 0.15 to 0.10 mm, you should therefore keep the flow constant or lower it slightly. When testing, only ever change one of the two values at a time.
Ironing Type: top surface only or all top surfaces?
On parts with many ledges, the “all top surfaces” setting irons every step – this takes time and is often unnecessary, because intermediate steps will not be visible later anyway. “Top surface only” irons exclusively the highest top surface. For a housing with one large visible surface, this is usually the best choice; for stepped front panels with several visible levels, choose “all top surfaces” instead. The “all solid surfaces” option additionally irons internal solid layers and only makes sense in special cases.
Ironing direction and pattern
Some slicers, such as OrcaSlicer, allow a separate angle for the ironing lines. In practice, an offset from the direction of the last top-layer lines often results in more even levelling, because the nozzle passes across the ridges rather than along them. On circular lids, the concentric pattern produces a record-like finish without kinks at the turning points.
5. Configuration in PrusaSlicer, OrcaSlicer, Bambu Studio & Cura
The feature has a similar name in all common slicers but is located in different places. Menu labels may differ slightly depending on version and language.
Bambu Studio & OrcaSlicer
Navigate to Quality > Ironing. Under Ironing Type, select “Top surfaces” (all top surfaces) or “Topmost surface” (the highest surface only). You can then set the pattern, Ironing flow and Ironing line spacing; OrcaSlicer additionally offers Ironing inset and an ironing angle. Depending on the version, you will find the ironing speed in the Speed tab. Proven starting values: flow 10–15 %, line spacing 0.10–0.15 mm, speed around 30 mm/s.
Handy: in both programs, ironing can be enabled per object or via modifiers for individual parts only. This way, on mixed build plates, the print time for purely functional parts stays unchanged.
PrusaSlicer
Under Print Settings > Infill > Ironing, tick Enable ironing (Expert mode required). The available ironing types are “All top surfaces”, “Topmost surface only” and “All solid surfaces”. Flow rate and spacing between ironing passes are set in the same block, the ironing speed under Speed. The defaults (around 15 % flow, 0.1 mm spacing, a rather low speed) already work well for PLA. Using “Add settings” via right-click, ironing can also be enabled for individual objects only.
Ultimaker Cura
In the Top/Bottom category (older versions: Shell), activate the Enable Ironing option; you may first need to make the settings visible via the setting visibility options. Iron Only Highest Layer restricts ironing to the topmost surface. Zig Zag and Concentric are available as patterns, and Monotonic Ironing Order ensures a uniform line order. Set Ironing Line Spacing to approx. 0.1 mm, Ironing Flow to 10–15 % and Ironing Inset to suit the line width.
Terminology overview: what is called what, and where?
| Function | PrusaSlicer | Bambu Studio / OrcaSlicer | Cura |
|---|---|---|---|
| Enable | Enable ironing (Infill) | Ironing Type ≠ “No ironing” (Quality) | Enable Ironing (Top/Bottom) |
| Top surface only | Ironing type “Topmost surface only” | Topmost surface | Iron Only Highest Layer |
| Ironing flow | Flow rate | Ironing flow | Ironing Flow |
| Line spacing | Spacing between ironing passes | Ironing line spacing | Ironing Line Spacing |
| Speed | Speed > Ironing | Ironing speed | Ironing Speed |
| Pattern | linear pattern (fixed) | Ironing pattern (Rectilinear / Concentric) | Ironing Pattern (Zig Zag / Concentric) |
6. Ironing calibration test: finding the right ironing flow
Instead of trying out values on a large part, it is worth doing a short test print with several flat test pieces. This lets you compare the settings side by side under identical conditions:
- Create test pieces: Place four to six flat squares (e.g. 20 × 20 × 3 mm) on the build plate. The surface should be large enough to assess differences in gloss properly.
- Assign one flow per object: Using per-object settings (PrusaSlicer, OrcaSlicer, Bambu Studio) or a modifier mesh (Cura), give each square a different ironing flow, e.g. 8 %, 10 %, 12 %, 14 % and 16 %.
- Keep all other values constant: Line spacing, speed, temperature and cooling remain the same for all samples.
- Evaluate: Look at the surfaces under raking light and run your fingernail across them. Visible ridges or holes mean too little flow; beads at the edge or a scaly texture mean too much.
- Fine-tune: Starting from the best square, vary the line spacing or speed in a second round.
Record the results for each filament and nozzle in the slicer profile. Even a change of brand or colour can require a slightly different ironing flow.
7. Material analysis: which filament delivers the best results?
Not every polymer reacts in the same way to heat treatment by the nozzle. The following overview summarises guideline values for a 0.4 mm nozzle; they are no substitute for your own calibration test:
| Material | Ironing Flow | Line spacing | Speed | Typical finish |
|---|---|---|---|---|
| PLA / Tough PLA / PLA Matte | 10 – 15 % | 0.10 – 0.12 mm | 20 – 40 mm/s (fast printers sometimes higher) | Very flat, satin matt to glossy |
| PETG | 8 – 12 % | 0.12 – 0.15 mm | 20 – 35 mm/s | Smooth and glossy, provided the nozzle is clean |
| ABS / ASA | 12 – 16 % | 0.10 – 0.12 mm | 25 – 40 mm/s | Homogeneous and dense, a good basis for further finishing |
| PA-CF / PETG-CF | 8 – 10 % (with limitations) | approx. 0.14 mm | 25 – 35 mm/s | A more uniform matt finish is possible, fibres may roughen – test first |
| TPU / flexible filaments | not recommended | – | – | Elastic material yields, uneven result |
- PLA: The most forgiving material. It melts cleanly and produces a homogeneous, satin matt to glossy finish. PLA Matte in particular benefits visibly, because otherwise the line structure makes the matt appearance look uneven. When ironing very slowly in enclosed printers, watch out for heat creep.
- PETG: Very good results, but PETG tends to stick to the nozzle and, if the flow is too high, to form material build-up (blobbing), which is then dragged across the surface. A low flow of 8–12 % and a clean nozzle are crucial.
- ABS & ASA: Iron well and produce dense, even surfaces. Print in an enclosed build chamber to avoid warping. An ironed surface is also a good starting point for subsequent chemical smoothing.
- Carbon fibre filaments (PA-CF, PETG-CF): Suitable with limitations. Ironing can make the matt carbon look more uniform, but fibres lying on the surface can also be roughened. Test on a sample surface beforehand. A hardened nozzle is a must, and the additional ironing passes increase nozzle wear.
- TPU (flexible): Not recommended. The elastic material yields under the nozzle, leading to juddering and uneven displacement.
8. Defects & solutions
Most ironing problems can be traced back to flow, line spacing, temperature or a dirty nozzle. The table helps with quick diagnosis:
| Defect | Cause | Solution |
|---|---|---|
| Rough edges, beads or burrs along the outlines | Displaced material is pushed over the outer edge; inset too small or flow too high | Increase Ironing Inset to approx. 0.35 mm; lower the flow in 2 % steps |
| Scaly, wavy surface | Ironing flow too high, especially in combination with small line spacing | Reduce the flow, e.g. from 15 % to 10–12 %, or increase the line spacing slightly |
| Glossy stripes with holes, visible residual ridges | Too little flow or line spacing too large; top layer already under-extruded | Raise the flow by 2–3 % or reduce the spacing from 0.15 to 0.10 mm; check the top-layer flow |
| Uneven matt and glossy patches | Fluctuating travel speed, changing line order or temperature fluctuations | Choose a constant speed of approx. 25–30 mm/s, use a monotonic pattern, keep cooling even |
| Nozzle tears the surface or leaves streaks | Dirty nozzle tip, flow too low or pillowing beneath the top layer | Clean the nozzle with a brass brush, increase the flow slightly, plan more top layers |
| Lumps of material on the surface (especially PETG) | Material accumulates on the nozzle and is wiped off | Lower the flow to 8–10 %, use a silicone sock, clean the nozzle before printing |
| Under-extrusion or clogging during long ironing phases | Heat creep due to low material throughput, especially with PLA in an enclosed build chamber | Open the chamber door or lid when printing PLA, check the hotend fan, do not set the nozzle temperature unnecessarily high |
| Sunken areas above the infill | Too few top layers, melted material sinks into cavities | Set 4–5 top layers or approx. 0.8 mm top shell, check infill density |
| Print time increases sharply | All top surfaces, including invisible steps, are ironed | Switch to “top surface only” or enable ironing per object/modifier only where it is visible |
9. Limits of ironing & sensible alternatives
Ironing works exclusively on horizontal, flat, upward-facing surfaces. Sloped surfaces, curves and side walls are not covered, because the nozzle only irons in one Z plane. Small islands, fine lettering and narrow webs hardly benefit either: there is often not enough room for clean ironing lines, and fine contours can smear.
Other approaches are better suited to such geometries:
- Stair-stepping on curves: Variable or adaptive layer heights reduce the stepping effect on curved surfaces.
- Visible seams on side walls: These are caused by the Z seam, not by the top layer – here, targeted placement or concealment of the Z seam helps.
- Surfaces smooth on all sides: Sanding, priming, painting or chemical smoothing for ABS and ASA – our guide to the surface finishing of 3D prints provides an overview.
- Finest details and an injection-moulded look: If surfaces need to be smooth on all sides, SLA printing is often a better choice than FDM with post-processing.
Ironing has practically no effect on part strength. If a part needs to be stiffer or more resilient, the number of walls and top layers are decisive – find out more in our guide to wall thickness & perimeters.
10. Time vs. quality: is ironing worth it?
The additional print time depends almost entirely on the size of the ironed top surfaces. On tall, slender parts with a small top face it is barely significant, whereas on large, flat plates ironing can account for a noticeable share – the tight line spacing means many lines per square centimetre. The slicer preview in PrusaSlicer, OrcaSlicer and Bambu Studio shows ironing as a separate line type including its share of the time, so you can estimate the extra effort precisely before printing.
This is offset by the elimination of manual finishing: where a top surface would otherwise have to be sanded, filled and painted, ironing is usually much cheaper and faster. For visible parts in rapid prototyping and small batches, the feature is therefore almost always worthwhile; for concealed functional parts, you can safely leave it out.
For industrial and development companies in Berlin Mitte, Berlin Charlottenburg and across Berlin, we manufacture visible parts with a suitable surface strategy – at short notice if required, via our express 3D printing service.
Need visible parts with a smooth surface?
Upload your STL or 3MF file, choose the process, material and quantity – the price is calculated instantly.
11. Frequently asked questions (FAQ)
Does ironing clog my nozzle?
With the correct settings, generally not, because around 10–15 % material is continuously extruded during ironing and the melt flow stays active. Due to the low throughput, however, heat creep can occur during long ironing phases, especially with PLA in enclosed printers. A nozzle temperature that is not too high and a properly working hotend fan help prevent this.
How much does ironing increase print time?
That depends almost solely on the size of the ironed top surfaces. For parts with a small top face, the extra effort is low; for large flat plates, it is clearly noticeable. The slicer preview shows ironing as a separate line type with its share of the time, so you can check the additional effort in advance.
Should I iron all top surfaces or only the topmost surface?
For parts with one large visible surface, “top surface only” is usually sufficient and saves time. For stepped front panels or housings with several visible levels, “all top surfaces” makes sense. Alternatively, ironing can be enabled selectively per object or modifier only where it is visible.
What layer height is ideal before ironing?
For the last top layer before ironing, 0.16 to 0.20 mm has proven effective, combined with 4–5 solid top layers or a top shell of around 0.8 mm. This prevents the melted material from sinking into the infill, and the ridges are shallow enough to be filled completely.
Can ironing be used with a concentric pattern?
Yes. OrcaSlicer, Bambu Studio and Cura offer a concentric ironing pattern. On round lids, it produces an even, record-like finish without kinks at the turning points. For rectangular surfaces, a linear pattern is usually more even.
Can sloped or curved surfaces be ironed?
No. Ironing only works on horizontal, flat, upward-facing surfaces. For curved surfaces, adaptive layer heights, sanding and painting, or switching to SLA printing if all sides need to be smooth, are the better options.
Does ironing work with carbon fibre filaments such as PA-CF?
With limitations. Ironing can make the matt carbon look more uniform, but fibres lying on the surface may also be roughened in the process. A test on a sample surface with a low flow of around 8–10 % is recommended. A hardened nozzle is a must, as the additional passes increase wear.
Which nozzle shape is best suited to ironing?
Nozzles with a wide, flat end face smooth best, because they have more contact area with the surface. Pointed, worn or damaged nozzle tips are more likely to leave streaks. The nozzle should be clean before printing so that no material residue is dragged across the surface.